首页 > 产品展示 > 材质特性 > Ni-Zn > K081 |
|
 |
| |
| |
■材质特性-K081 |
|
| |
|
|
| |
Symbol |
Unit |
Measuring Conditions |
Low loss Material |
| |
|
|
Freq. |
Flux den. |
Temp. |
K081 |
K12 |
| Initial Permeability |
μi |
|
|
|
25°C |
800± 25% |
1200± 25% |
| Power Loss |
Pv |
KW/m3 |
50kHz |
150mT |
25°C |
400 |
315 |
| 100°C |
300 |
270 |
| 120°C |
295 |
287 |
| Saturation Flux Density |
Bms |
mT |
1kHz |
H = 1200A/m |
25°C |
410 |
355 |
| Remanence |
Brms |
mT |
1kHz |
H = 1200A/m |
25°C |
272 |
250 |
| Coercivity |
Hc |
A/m |
1kHz |
H = 1200A/m |
25°C |
27 |
17 |
| Curie Temperature |
Tc |
°C |
|
|
|
>190 |
>160 |
| Resistivity |
ρ |
Ωm |
|
|
|
>106 |
>106 |
| Density |
d |
g/cm3 |
|
|
|
5.10 |
5.10 |
|
| |
|